REVIEW 3 major objections 5 minor 81 references
Hydrogen-induced fast fracture in a 1.5 GPa dual-phase steel
T0 review · 3 major / 5 minor · reviewed 2026-08-15 · deepseek-v4-flash
Pith's one-line read Hydrogen embrittlement in a 1.5 GPa dual-phase steel is governed by a crack-velocity threshold, not by hydrogen acting at the crack tip.
desk verdict First site-specific TEM/TKD evidence of ferrite blunting then {100} cleavage in a 1.5 GPa DP steel, wrapped in a plausible but unmeasured HIFF story. read the letter →
The pith
A machine-rendered reading of the paper's core claim, the machinery that carries it, and where it could break.
The reading
What carries the argument
The central mechanism is the hydrogen-induced fast-fracture (HIFF) model, applied in two stages. In stage A, hydrogen diffuses to prior austenite grain boundaries, weakens them by hydrogen-enhanced decohesion, and sustains fast brittle crack growth in martensite through continued hydrogen supply to the crack tip. In stage B, once the crack velocity exceeds the critical threshold Vcrit ≈ 5.4 m/s for BCC iron, the high crack-tip strain rate prevents effective blunting by dislocation emission, so {100} ferrite cleavage persists even after hydrogen at the tip is exhausted. The paper modifies the original HIFF picture by replacing hydride-assisted crack initiation with hydrogen-enhanced decohesion at grain boundaries, and it uses the velocity threshold to explain why ferrite arrests short cracks but cleaves after long crack growth.
What would settle it
Directly measure the running crack velocity during the stage where ferrite cleaves on {100}, for example by high-speed imaging, electrical potential drop, or acoustic emission, in a hydrogen-precharged tensile specimen. If the crack is moving slower than about 5.4 m/s while {100} cleavage continues after hydrogen depletion, the central claim fails; the same test should also confirm that hydrogen is actually depleted at the crack tip at that moment.
Extended reading notes
Core claim
The paper reports that hydrogen pre-charging to 3.8 mass ppm diffusible hydrogen makes a 1.5 GPa dual-phase steel fracture at 900 MPa with only 0.57% elongation, well inside the elastic regime. The fracture path begins with intergranular cracking along prior austenite grain boundaries, attributed to hydrogen-enhanced decohesion assisted by hydrogen diffusion during loading. Ferrite blunts sub-surface cracks during initiation and early growth, but after significant crack propagation the same ferrite undergoes {100} cleavage, as identified by site-specific transmission electron microscopy and transmission Kikuchi diffraction. The authors propose that hydrogen-assisted crack growth in martensite accelerates the crack beyond a critical velocity, Vcrit ≈ 5.4 m/s for BCC iron; above this speed, crack-tip blunting by dislocation emission is suppressed, so brittle {100} ferrite cleavage can continue even after the hydrogen supply to the crack tip is depleted. The river-pattern serrations on the {100} surface are explained by crack deflection along {110} micro deformation bands and {121} twins, with the connecting surfaces being non-crystallographic coalescence features.
Load-bearing premise
The crack actually runs faster than the critical velocity (roughly 5.4 m/s for body-centred cubic iron), a value inferred from fracture morphology and the model rather than measured; if the local crack speed stays below that threshold, the proposed explanation for sustained brittle cleavage after hydrogen depletion collapses.
Editorial extensions
If this is right
- A ductile ferrite phase does not guarantee hydrogen resistance: ferrite arrests cracks only while the crack is short and its velocity is below the critical threshold.
- In a hydrogen-precharged specimen, brittle fracture can begin within the elastic regime at 900 MPa, so design margins for high-strength steels must account for fast-fracture initiation at prior austenite grain boundaries.
- Strain-rate sensitivity of hydrogen embrittlement in this steel can be understood through hydrogen diffusion kinetics to grain boundaries rather than through hydride formation at cavities.
- The {100} ferrite cleavage surface forms river-pattern serrations by crack deflection along {110} micro deformation bands and {121} twins; the connecting surfaces are non-crystallographic coalescence features.
- Microstructure design should aim to disrupt the continuous martensite network and trap diffusible hydrogen, for example through carbides, fine MnS inclusions, or Cu precipitates, so the crack never reaches the critical velocity.
Reading between the lines
- If the velocity threshold is the real controlling parameter, then the same ferrite grain can act as an arrestor early in fracture and as a cleavage path later; the crack length at which ferrite switches roles should be predictable from applied stress and the threshold, which could be mapped experimentally.
- Direct crack-speed measurement in similar pre-charged high-strength steels would test whether the inferred threshold is real; observing {100} cleavage below roughly 5.4 m/s would force an alternative explanation.
- The HIFF picture implies that trapping strategies that only remove diffusible hydrogen may not stop fast fracture once the crack is long; what matters is preventing the crack from ever reaching the critical velocity.
- Because the model replaces hydride-assisted initiation with hydrogen-enhanced decohesion at prior austenite grain boundaries, steels with engineered grain-boundary segregation would be predicted to raise the stress needed to cross the threshold; this is testable.
Signed reviews
Editorial analysis
A structured set of objections, weighed in public.
Referee Report
Summary. The paper reports an experimental study of hydrogen embrittlement in a 1.5 GPa ferrite-martensite dual-phase (DP) steel. Hydrogen pre-charging to 3.8 mass ppm diffusible hydrogen, followed by slow strain-rate tensile testing at 10^-4 s^-1, produces fracture within the elastic regime at 900 MPa. Fractography, site-specific TEM/TKD, and EBSD reveal: surface crack initiation at prior austenite grain boundaries with intergranular and quasi-cleavage features; ferrite blunting and crack arrest near the initiation region; mixed-mode fracture ahead of initiation; and predominantly brittle {100} ferrite cleavage after significant crack growth. The authors interpret these observations using the hydrogen-induced fast fracture (HIFF) model of Shishvan et al., replacing the hydride sub-mechanism with hydrogen-enhanced decohesion at PAGBs, and propose that once the crack velocity exceeds Vcrit = 5.4 m/s, cleavage in ferrite persists even after hydrogen depletion at the crack tip. They also propose a mechanism for river-pattern formation via crack deflection along {110} micro-deformation bands and {121} twins.
Significance. If the central claim is correct, the work identifies a qualitatively important regime for hydrogen embrittlement in DP steels: ferrite's crack-arresting ability is effective only for short cracks, and long-crack propagation is governed by fast fracture rather than by direct hydrogen-assisted crack-tip processes. The experimental dataset is rich and internally consistent; the HIFF interpretation is applied without fitting parameters, and the proposed river-pattern mechanism is falsifiable. However, the load-bearing assertion that the local crack velocity actually exceeds the literature value of Vcrit is not directly measured, so the significance depends on whether the authors can strengthen this inference with quantitative analysis or a direct velocity measurement.
major comments (3)
- [Section 4.4] The central stage-B claim is supported only by an unmeasured crack velocity. The authors infer v > Vcrit = 5.4 m/s from the monotonic relation K ∝ (crack length)^0.5, but this establishes only that K and hence a characteristic crack speed increase with crack length; it does not establish that the local crack speed exceeds the BCC-Fe threshold at the crack length where {100} ferrite cleavage first appears (Figs. 5 and 6). The observed transition from mixed-mode to predominantly brittle fracture is also consistent with an increasing crack-tip driving force and constraint with crack growth, which would occur with or without hydrogen assistance. To make stage-B load-bearing, the authors should either measure the crack speed (e.g., by potential drop, acoustic emission, or high-speed imaging) or provide a quantitative fracture-mechanics estimate of the local stress intensity at the transition crack length and show that it is sufficient to drive ferrite cleavage under the observed 900 MPa nominal stress. Without this, the sustained {100} cleavage after hydrogen depletion could be caused by the crack-length-dependent stress state rather than by v > Vcrit.
- [Section 4.4] The exclusion of the stress-partitioning mechanism is not quantitative. The authors argue that the high strain rate at the crack tip cannot be due to stress partitioning because the hydrogen-charged specimen fails at a nominal stress of 900 MPa, whereas the uncharged specimen's cleavage was attributed to partitioning with martensite stresses of ~1700 MPa. However, crack-tip fields scale with the stress intensity factor, not with the nominal stress alone; a long crack at 900 MPa can produce a larger K than a short crack at 1700 MPa, and the authors themselves use this K scaling for the velocity argument. The authors should estimate the local K at the observed mixed-to-cleavage transition and show that the resulting crack-tip strain rates are below those required for cleavage unless HIFF is invoked. In addition, the high dislocation density observed beneath the {100} cleavage (Section 3.4, Fig. 9a) indicates substantial plasticity, which the HIFF model must accommodate; the paper should specify how much dislocation emission is compatible with v > Vcrit in the Shishvan framework.
- [Section 4.3] The proposed stage-A hydrogen supply mechanism is in tension with the paper's own diffusion argument. Section 4.2 states that at brittle crack speeds (~1000 m/s) hydrogen cannot diffuse ahead of the crack tip over relevant distances, and Section 4.3 replaces Shishvan's hydride-assisted growth with hydrogen diffusion to the PAGB crack tip to sustain v > Vcrit. The authors should clarify whether the hydrogen that sustains stage A is pre-existing at the PAGB (accumulated during the loading phase) or must arrive by diffusion during crack growth. If it must arrive by diffusion, the paper should quantify the hydrogen-enriched zone size and show that it can sustain the intergranular crack path at high velocity; if it is pre-existing, the length of the PAGB segment over which stage A operates should be specified so that the transition to stage B can be identified. Currently this transition is not tied to any measured microstructural length.
minor comments (5)
- [Section 3.2 and Fig. 2] The uncharged specimen is tested only at 10^-3 s^-1, so the charged 10^-4 s^-1 test is compared without a corresponding uncharged baseline at the same strain rate. Consider adding an uncharged 10^-4 s^-1 test or discussing this limitation explicitly.
- [Fig. S2 caption] There is a typo in the caption: 'Prescence' should be 'Presence'.
- [Figures 8 and 9] The prime notation for subfigures (e.g., Fig. 8f' and Fig. 9f') is nonstandard; the authors should define the prime notation in the captions or use separate labels to avoid ambiguity.
- [Table 2] The table has empty cells for crack initiation in some columns; consider filling them with 'not observed' or a dash to avoid implying missing data.
- [Section 3.2] The paper does not report the hydrogen content after the tensile test; since slow strain-rate tests take time, some hydrogen may desorb during loading. State whether the 3.8 mass ppm is the pre-test content and discuss possible loss.
Circularity Check
No significant circularity: the HIFF interpretation adapts an external model (Shishvan et al.) to new fractographic and TEM observations, with no fitted parameter relabeled as a prediction.
full rationale
The paper's causal chain is experimental observation -> mechanism hypothesis, not input -> derived output. Crack initiation at PAGBs via HEDE is supported by EBSD, fractography, and independent hydrogen-diffusion literature, not by the conclusion it feeds. The central velocity threshold, Vcrit = 5.4 m/s for BCC Fe, is imported from Shishvan et al. [52], an external model, and is not fitted to any quantity in this paper. The absence of a direct crack-velocity measurement is a genuine evidentiary gap and a correctness risk, but it is not circularity: the model is not calibrated to the observed {100} ferrite cleavage, and the observed morphology is not the definition of the model. Self-citations [33] and [5] supply prior baselines (uncharged tensile behavior and U-bend delayed fracture) and are not the sole load-bearing justification for the HIFF claim; the paper's own site-specific TEM and TKD show ferrite blunting at initiation and {100} cleavage after significant growth. The exclusion of stress partitioning as the cause of the high crack-tip strain rate is an empirical argument based on prior stress-partitioning values and the current low nominal failure stress, not a restatement of the model. No equation in the paper reduces to its own inputs, and no fitted parameter is renamed as a prediction. The river-pattern mechanism is explicitly offered as a plausible hypothesis requiring further theoretical validation, so it does not close a circular loop. Overall, the derivation is self-contained against external model parameters and experimental observations, and no circular step can be exhibited.
Assumptions & free parameters
assumptions (4)
- domain assumption The HIFF model of Shishvan et al. [52] describes hydrogen-assisted fast fracture in BCC Fe with a critical velocity Vcrit of about 5.4 m/s below which dislocation emission blunts the crack.
- domain assumption Hydrogen diffusion distances at room temperature of 10^-4 to 10^-6 m in 1 s [50, 51] are too small for hydrogen to reach the crack tip during fast fracture, so the {100} ferrite cleavage is not directly hydrogen assisted.
- domain assumption The uncharged 1.5 GPa DP steel exhibits the same microstructure and {100} ferrite cleavage under tensile loading as reported in the authors' prior study [33].
- standard math Standard EBSD trace analysis and KAM maps reliably identify cleavage planes and strain localization in the ferrite and martensite phases.
Cite this review
Pith. "Pith review of Hydrogen-induced fast fracture in a 1.5 GPa dual-phase steel." pith.science (2026). https://pith.science/paper/ITOMGJRQ
@misc{pith2026250906323,
author = {Pith},
title = {Pith review of: Hydrogen-induced fast fracture in a 1.5 GPa dual-phase steel},
year = {2026},
howpublished = {\url{https://pith.science/paper/ITOMGJRQ}},
note = {Machine review of arXiv:2509.06323}
}
read the original abstract
This study clarifies the hydrogen embrittlement (HE) behavior in a 1.5 GPa ferrite-martensite dual-phase (DP) steel. Hydrogen pre-charging (3.8 mass ppm diffusible hydrogen), followed by slow strain tensile testing (10-4 s-1), resulted in a brittle fracture at 900 MPa within the elastic regime. Fractographic studies indicated that surface crack initiation consists of intergranular and quasi-cleavage morphology; site-specific transmission electron microscopy (TEM) investigations revealed sub-surface secondary crack blunting by ferrite. A mixed-mode morphology consisting of ductile and brittle features was observed adjacent to crack initiation. It differs from the previous investigation of uncharged DP steel, wherein a predominant brittle fracture was observed. Following significant crack growth, the pre-charged specimen exhibited predominant brittle fracture; site-specific TEM and transmission Kikuchi diffraction studies revealed {100} ferrite cleavage cracking. Electron backscatter diffraction studies were performed on the cross-sectional cracks. We explain the HE via hydrogen-induced fast fracture mechanism. During loading, hydrogen diffuses to the prior austenite grain boundary, resulting in hydrogen-induced decohesion. Subsequent hydrogen diffusion to the crack tip promotes brittle fracture at high crack velocity (>Vcrit). The high crack velocity effectively inhibits crack blunting via dislocation emission, ensuring sustained brittle crack growth even after hydrogen depletion at the crack tip, resulting in {100} ferrite cleavage cracking. Based on TEM observations, we explain the formation of river pattern features on the {100} cleavage surface.
Reference graph
Works this paper leans on
-
[1]
Trapping of diffusible hydrogen via second-phase parƟcles such as carbides, carbonitrides, and copper precipitates [10–16]
-
[2]
The propensity of hydrogen-induced grain boundary cracking is dependent on the structure of the boundary (or the parent austenite boundary in the case of martensiƟc steels) [17,18]. Hence, a grain boundary engineering (GBE) approach via the increase in the fracƟon of low-energy boundaries (or special boundaries) enhances resistance to hydrogen embriƩlemen...
-
[3]
Hydrogen-enhanced decohesion (HEDE) is one of the dominant hydrogen embriƩlement mechanisms [21,22]. For example, in martensiƟc steels, hydrogen-induced intergranular cracking occurs along the prior austenite grain boundaries (PAGBs) [18,23,24]. Grain boundary segregaƟon engineering (GBSE) via segregaƟon of alloying elements such as Mo [25] and B [26] to ...
-
[4]
Grain refinement, for instance, in martensiƟc steels [27–29], has been reported to miƟgate hydrogen embriƩlement. Recently, Pinson et al. [30] designed martensiƟc steels with ferriƟc microfilm at the PAGBs to exploit the crack-arresƟng ability of ducƟle ferrite and achieved a 100% increase in the ducƟlity in the absence of hydrogen. However, in the presence...
-
[5]
Surface crack iniƟaƟon wherein the fracture surface consists of intergranular fracture and quasi- cleavage fracture features
-
[6]
Crack growth iniƟally occurs towards the center from the surface (across the thickness). Subsequently, the crack propagates across the width of the tensile specimen, from one end of the tensile specimen to the other
-
[7]
We examined the fracture surface aŌer significant crack propagaƟon along the width of the specimen. The local fracture at the center of the specimen (along the thickness) is predominantly briƩle, and the local fracture mode at the area adjacent to the shear lip was mixed-mode with both briƩle fracture features and ducƟle dimples. 10 Figure 7 (a) Site-speci...
-
[8]
Q. Liu, Q. Zhou, J. Venezuela, M. Zhang, A. Atrens, Hydrogen influence on some advanced high-strength steels, Corrosion Science 125 (2017) 114–138. hƩps://doi.org/10.1016/j.corsci.2017.06.012
Show all 81 references
-
[9]
Crack initiation region Significant crack growth Crack initiation region Significant crack growth Crack Initiation PAGB - Crack arrest X X X X X ✓ X ✓ Crack Propagation {110} + others QC {110} + {100} - {110} {100} Crack blunting {100} Crack blunting Table 2 summarizes the cra...
-
[10]
Ferrite helps arrest the cracks during their iniƟaƟon. Thus, the inability of ferrite to prevent HIFF can be ascribed to its low phase fracƟon which fails to disrupt the conƟnuous hard martensite network, thereby allowing crack propagaƟon within the martensite. Increasing the ...
-
[11]
Kim et al
A counterintuiƟve strategy is to engineer microstructures with a large volume fracƟon of sub-micron MnS inclusions. Kim et al. [68] have shown that fine or Ti(C,N)–MnS complex inclusions trap diffusible hydrogen effecƟvely in a 2 GPa martensiƟc steel. The S or S–Ti added steels e...
-
[12]
AlternaƟvely, the Cu present in steels recycled from scrap [69] can be used to produce nano-scale Cu precipitates to simultaneously induce precipitaƟon strengthening [70] and trap diffusible hydrogen [12]. 24 5 Conclusions This work provides the first insight into the effect of i...
-
[13]
X. Hu, Z. Feng, Advanced High-Strength Steel - Basics and ApplicaƟons in the AutomoƟve Industry, 2021. hƩps://doi.org/10.2172/1813170
2021 doi
-
[15]
hƩps://www.oecd-ilibrary.org/energy/co2-emissions-from-fuel-combusƟon-2019_2a701673-en 25 (accessed August 8, 2022)
OECD, CO2 Emissions from Fuel CombusƟon 2019, OrganisaƟon for Economic Co-operaƟon and Development, Paris, 2019. hƩps://www.oecd-ilibrary.org/energy/co2-emissions-from-fuel-combusƟon-2019_2a701673-en 25 (accessed August 8, 2022)
2019
-
[16]
H. Fu, W. He, Z. Mi, Y. Yan, J. Zhang, J. Li, Effects of heterogeneous plasƟc strain on hydrogen-induced cracking of twinning-induced plasƟcity steel: A quanƟtaƟve approach, Corrosion Science 209 (2022) 110782. hƩps://doi.org/10.1016/j.corsci.2022.110782
2022
-
[17]
Varanasi, M
R.S. Varanasi, M. Koyama, Y . Shibayama, S. Chiba, S. Ajito, T. Hojo, E. Akiyama, Hydrogen-Induced Delayed Fracture in a 1.5 GPa Dual-Phase Steel via Coalescence of Surface and Sub-surface Cracks, Metall Mater Trans A 54 (2023) 2989–2997. hƩps://doi.org/10.1007/s11661-023-07096-8
2023 doi
-
[18]
Momotani, A
Y . Momotani, A. Shibata, N. Tsuji, Hydrogen embriƩlement behaviors at different deformaƟon temperatures in as-quenched low-carbon martensiƟc steel, InternaƟonal Journal of Hydrogen Energy 47 (2022) 3131–3140. hƩps://doi.org/10.1016/j.ijhydene.2021.10.169
2022 doi
-
[19]
S. Li, E. Akiyama, N. Uno, K. Hirai, K. Tsuzaki, B. Zhang, EvaluaƟon of delayed fracture property of outdoor- exposed high strength AISI 4135 steels, Corrosion Science 52 (2010) 3198–3204. hƩps://doi.org/10.1016/j.corsci.2010.05.038
2010 doi
-
[21]
Lovicu, M
G. Lovicu, M. BoƩazzi, F. D’ Aiuto, M. De SancƟs, A. DimaƩeo, C. Santus, R. ValenƟni, Hydrogen EmbriƩlement of AutomoƟve Advanced High-Strength Steels, Metall Mater Trans A 43 (2012) 4075–4087. hƩps://doi.org/10.1007/s11661-012-1280-8
2012 doi
-
[22]
P .-Y . Liu, B. Zhang, R. Niu, S.-L. Lu, C. Huang, M. Wang, F. Tian, Y. Mao, T. Li, P .A. Burr, H. Lu, A. Guo, H.-W. Yen, J.M. Cairney, H. Chen, Y.-S. Chen, Engineering metal-carbide hydrogen traps in steels, Nat Commun 15 (2024)
2024
-
[23]
Mohrbacher, T
H. Mohrbacher, T. Senuma, Alloy OpƟmizaƟon for Reducing Delayed Fracture SensiƟvity of 2000 MPa Press Hardening Steel, Metals 10 (2020) 853. hƩps://doi.org/10.3390/met10070853
2020 doi
-
[24]
Vandewalle, T
L. Vandewalle, T. Depover, K. Verbeken, Current state-of-the-art of hydrogen trapping by carbides: From theory to experiment, Interna Ɵonal Journal of Hydrogen Energy (2024). hƩps://doi.org/10.1016/j.ijhydene.2024.03.266
2024 doi
-
[25]
McCarroll, Y.-C
I.E. McCarroll, Y.-C. Lin, A. Rosenthal, H.-W . Yen, J.M. Cairney, Hydrogen trapping at dislocaƟons, carbides, copper precipitates and grain boundaries in a dual precipitaƟng low-carbon martensiƟc steel, Scripta Materialia 221 (2022) 114934. hƩps://doi.org/10.1016/j.scriptamat...
2022
-
[26]
Takahashi, K
J. Takahashi, K. Kawakami, T. Tarui, Direct observaƟon of hydrogen-trapping sites in vanadium carbide precipitaƟon steel by atom probe tomography, Scripta Materialia 67 (2012) 213–216. hƩps://doi.org/10.1016/j.scriptamat.2012.04.022
2012 doi
-
[27]
Y.-S. Chen, D. Haley, S.S.A. Gerstl, A.J. London, F. Sweeney, R.A. Wepf, W.M. Rainforth, P .A.J. Bagot, M.P . Moody, Direct observaƟon of individual hydrogen atoms at trapping sites in a ferriƟc steel, Science 355 (2017) 1196–
2017
-
[28]
Fuchigami‡, H
H. Fuchigami‡, H. Minami§, M. Nagumo∥, Effect of grain size on the suscepƟbility of martensiƟc steel to hydrogen-related failure, Philosophical Magazine Le Ʃers 86 (2006) 21 –29. hƩps://doi.org/10.1080/09500830500482316
2006 doi
-
[30]
Hammer, L
P . Hammer, L. Romaner, V.I. Razumovskiy, Hydrogen trapping in mixed carbonitrides, Acta Materialia 268 (2024) 119754. hƩps://doi.org/10.1016/j.actamat.2024.119754
2024
-
[31]
Shibata, I
A. Shibata, I. GuƟerrez-UrruƟa, A. Nakamura, K. Okada, G. Miyamoto, Y . Madi, J. Besson, T. Hara, K. Tsuzaki, 26 Three-dimensional propagaƟon behavior of hydrogen-related intergranular cracks in high-strength martensiƟc steel, InternaƟonal Journal of Hydrogen Energy 48 (2023) ...
2023 doi
-
[32]
J.H. Kim, G. Miyamoto, A. Shibata, T. Hojo, M. Koyama, Y . Zhang, T. Furuhara, Influence of austenite grain boundary misorientaƟon on hydrogen-induced intergranular crack propagaƟon in a medium carbon martensiƟc steel, Acta Materialia 274 (2024) 120036. hƩps://doi.org/10.1016/j...
2024
-
[33]
Kwon, S.-P
Y.J. Kwon, S.-P . Jung, B.-J. Lee, C.S. Lee, Grain boundary engineering approach to improve hydrogen embriƩlement resistance in FeMnC TWIP steel, InternaƟonal Journal of Hydrogen Energy 43 (2018) 10129– 10140. hƩps://doi.org/10.1016/j.ijhydene.2018.04.048
2018 doi
-
[34]
Kwong, W .Y
W.Y . Kwong, W .Y. Zhang, Electron-beam assisted plaƟnum deposiƟon as a protecƟve layer for FIB and TEM applicaƟons, in: ISSM 2005, IEEE InternaƟonal Symposium on Semiconductor Manufacturing, 2005., 2005: pp. 469–471. hƩps://doi.org/10.1109/ISSM.2005.1513408
2005
-
[35]
Koyama, C.C
M. Koyama, C.C. Tasan, E. Akiyama, K. Tsuzaki, D. Raabe, Hydrogen-assisted decohesion and localized plasƟcity in dual-phase steel, Acta Materialia 70 (2014) 174–187. hƩps://doi.org/10.1016/j.actamat.2014.01.048
2014 doi
-
[36]
Djukic, G.M
M.B. Djukic, G.M. Bakic, V. Sijacki Zeravcic, A. Sedmak, B. Rajicic, The synergisƟc acƟon and interplay of hydrogen embriƩlement mechanisms in steels and iron: Localized plasƟcity and decohesion, Engineering Fracture Mechanics 216 (2019) 106528. hƩps://doi.org/10.1016/j.engfra...
2019
-
[37]
F. Dong, J. Venezuela, H. Li, Z. Shi, Q. Zhou, L. Chen, J. Chen, L. Du, A. Atrens, The influence of phosphorus on the temper embriƩlement and hydrogen embriƩlement of some dual-phase steels, Materials Science and Engineering: A 854 (2022) 143379. hƩps://doi.org/10.1016/j.msea.2...
2022
-
[38]
T. Chen, M. Koyama, T. Chiba, E. Akiyama, K. Takai, Mesoscale quanƟficaƟon of grain boundary character and local plasƟcity in hydrogen-assisted intergranular and intergranular-like cracking paths in tempered martensiƟc steel, Materials Science and Eng ineering: A 886 (2023) 145...
2023
-
[39]
Yoo, M.C
J. Yoo, M.C. Jo, M.C. Jo, S. Kim, S.-H. Kim, J. Oh, S.S. Sohn, S. Lee, Effects of solid soluƟon and grain-boundary segregaƟon of Mo on hydrogen embriƩlement in 32MnB5 hot-stamping steels, Acta Materialia 207 (2021) 116661. hƩps://doi.org/10.1016/j.actamat.2021.116661
2021
-
[40]
Hachet, A
G. Hachet, A. Tehranchi, H. Shi, M. Prabhakar, S. Wei, K. Angenendt, S. Zaefferer, B. Gault, B. Sun, D. Ponge, D. Raabe, SegregaƟon at prior austenite grain boundaries: The compeƟƟon between boron and hydrogen, InternaƟonal Journal of Hydrogen Energy 95 (2024) 734–746. hƩps://d...
2024 doi
-
[41]
Cho, P .E
L. Cho, P .E. Bradley, D.S. Lauria, M.J. Connolly, E.J. Seo, K.O. Findley, J.G. Speer, L. Golem, A.J. SliŅa, Effects of hydrogen pressure and prior austenite grain size on the hydrogen embriƩlement characterisƟcs of a press- hardened martensiƟc steel, InternaƟonal Journal of Hy...
2021 doi
-
[42]
Marơnez-Pañeda, S
E. Marơnez-Pañeda, S. del Busto, C.F. Niordson, C. Betegón, Strain gradient plasƟcity modeling of hydrogen diffusion to the crack Ɵp, InternaƟonal Journal of Hydrogen Energy 41 (2016) 10265–10274. hƩps://doi.org/10.1016/j.ijhydene.2016.05.014
2016 doi
-
[43]
Kimura, S
Y. Kimura, S. Takagi, T. Hara, S. Terasaki, K. Tsuzaki, Hydrogen-induced delayed fracture of a martensiƟc steel with fine prior-austenite grain size, J. Phys. IV France 112 (2003) 403–406. 27 hƩps://doi.org/10.1051/jp4:2003911
2003 doi
-
[44]
Pinson, S.M
M. Pinson, S.M. Das, H. Springer, T. Depover, K. Verbeken, The addiƟon of aluminum to briƩle martensiƟc steels in order to increase ducƟlity by forming a grain boundary ferriƟc microfilm, Scripta Materialia 213 (2022) 114606. hƩps://doi.org/10.1016/j.scriptamat.2022.114606
2022
-
[45]
Pinson, H
M. Pinson, H. Springer, K. Verbeken, T. Depover, The effect of an Al-induced ferriƟc microfilm on the hydrogen embriƩlement mechanism in martensiƟc steels, Materials Science and Engineering: A 851 (2022) 143587. hƩps://doi.org/10.1016/j.msea.2022.143587
2022
-
[46]
The already briƩle PAGBs (given they crack in the uncharged specimen [33]) would readily undergo enhanced decohesion due to hydrogen accumulaƟon during tensile loading
due to microscopic stress-induced diffusion during loading [47]. The already briƩle PAGBs (given they crack in the uncharged specimen [33]) would readily undergo enhanced decohesion due to hydrogen accumulaƟon during tensile loading. Notably, no decohesion of the ferrite-marten...
-
[47]
Tasan, M
C.C. Tasan, M. Diehl, D. Yan, M. Bechtold, F. Roters, L. Schemmann, C. Zheng, N. Peranio, D. Ponge, M. Koyama, K. Tsuzaki, D. Raabe, An Overview of Dual-Phase Steels: Advances in Microstructure-Oriented Processing and Micromechanically Guided Design, Annu. Rev. Mater. Res. 45 ...
2015 doi
-
[48]
Varanasi, M
R.S. Varanasi, M. Koyama, Y. Shibayama, E. Akiyama, Mixed type briƩle fracture in 1.5 GPa dual-phase steel via 100 ferrite cleavage cracking, Materials Science and Engineering: A (2022) 144021. hƩps://doi.org/10.1016/j.msea.2022.144021
2022
-
[49]
Schaffer, B
M. Schaffer, B. Schaffer, Q. Ramasse, Sample preparaƟon for atomic-resoluƟon STEM at low voltages by FIB, Ultramicroscopy 114 (2012) 62–71. hƩps://doi.org/10.1016/j.ultramic.2012.01.005
2012 doi
-
[50]
Drexler, B
A. Drexler, B. Helic, Z. Silvayeh, K. Mraczek, C. Sommitsch, J. Domitner, The role of hydrogen diffusion, trapping and desorpƟon in dual phase steels, J Mater Sci 57 (2022) 4789–4805. hƩps://doi.org/10.1007/s10853-021- 06830-0
2022 doi
-
[51]
Y . He, Y . Li, C. Chen, H. Yu, Diffusion coefficient of hydrogen intersƟƟal atom in α-Fe, γ-Fe and ε-Fe crystals by first-principle calculaƟons, InternaƟonal Journal of Hydrogen Energy 42 (2017) 27438–27445. hƩps://doi.org/10.1016/j.ijhydene.2017.08.212
2017 doi
-
[52]
Asari, S
D. Asari, S. Mizokami, M. Fukahori, K. Takai, Microscopic defects formed during crack incubaƟon, iniƟaƟon and propagaƟon processes causing hydrogen-related fracture of dual-phase steels, Materials Science and Engineering: A 780 (2020) 139209. hƩps://doi.org/10.1016/j.msea.2020.139209
2020
-
[53]
Ronevich, J.G
J.A. Ronevich, J.G. Speer, D.K. Matlock, J.A. Ronevich, J.G. Speer, D.K. Matlock, Hydrogen EmbriƩlement of Commercially Produced Advanced High Strength Sheet Steels, SAE InternaƟonal Journal of Materials and Manufacturing 3 (2010) 255–267. hƩps://doi.org/10.4271/2010-01-0447
2010 doi
-
[56]
Shishvan, G
S.S. Shishvan, G. Csányi, V.S. Deshpande, Strain rate sensiƟvity of the hydrogen embriƩlement of ferriƟc steels, Acta Materialia 257 (2023) 119173. hƩps://doi.org/10.1016/j.actamat.2023.119173
2023
-
[57]
Depover, S
T. Depover, S. Hertelé, K. Verbeken, The effect of hydrostaƟc stress on the hydrogen induced mechanical degradaƟon of dual phase steel: A combined experimental and numerical approach, Engineering Fracture Mechanics 221 (2019) 106704. hƩps://doi.org/10.1016/j.engfracmech.2019.106704
2019
-
[58]
Morooka, O
S. Morooka, O. Umezawa, S. Harjo, K. Hasegawa, Y . Toji, QuanƟtaƟve Analysis of Tensile DeformaƟon Behavior by In-Situ Neutron DiffracƟon for Ferrite-Martensite Type Dual-Phase Steels, Tetsu-to-Hagane 98 (2012) 311–
2012
-
[59]
MarƟn, J.A
M.L. MarƟn, J.A. Fenske, G.S. Liu, P . Sofronis, I.M. Robertson, On the formaƟon and nature of quasi-cleavage fracture surfaces in hydrogen embriƩled steels, Acta Materialia 59 (2011) 1601–1606. hƩps://doi.org/10.1016/j.actamat.2010.11.024
2011 doi
-
[60]
T. Chen, T. Chiba, M. Koyama, E. Akiyama, K. Takai, Factors DisƟnguishing Hydrogen-Assisted Intergranular and Intergranular-Like Fractures in a Tempered Lath MartensiƟc Steel, Metall Mater Trans A 53 (2022) 1645–1658. hƩps://doi.org/10.1007/s11661-022-06608-2
2022 doi
-
[61]
Momotani, A
Y . Momotani, A. Shibata, D. Terada, N. Tsuji, Effect of strain rate on hydrogen embriƩlement in low-carbon martensiƟc steel, Interna Ɵonal Journal of Hydrogen Energy 42 (2017) 3371 –3379. hƩps://doi.org/10.1016/j.ijhydene.2016.09.188
2017 doi
-
[62]
Okuno, K
K. Okuno, K. Takai, ExtracƟon of reversible hydrogen trapped on prior austenite grain boundaries and promoƟng intergranular fracture in the elasƟc region of tempered martensiƟc steel by uƟlizing frozen-in hydrogen distribuƟon at -196 °C, Acta Materialia 259 (2023) 119291. hƩps...
2023
-
[63]
Okada, A
K. Okada, A. Shibata, W. Gong, N. Tsuji, Effect of hydrogen on evoluƟon of deformaƟon microstructure in low- carbon steel with ferrite microstructure, Acta Materialia 225 (2022) 117549. hƩps://doi.org/10.1016/j.actamat.2021.117549
2022
-
[64]
Hudson, M
G. Hudson, M. Greenfield, The Speed of PropagaƟon of BriƩle Cracks in Steel, Journal of Applied Physics 18 (1947) 405–407. hƩps://doi.org/10.1063/1.1697664
1947 doi
-
[65]
Z. Wang, J. Liu, F. Huang, Y. Bi, S. Zhang, Hydrogen Diffusion and Its Effect on Hydrogen EmbriƩlement in DP Steels With Different Martensite Content, Front. Mater. 7 (2020). hƩps://doi.org/10.3389/fmats.2020.620000
2020
-
[66]
Barik, S
R.K. Barik, S. Biswal, K.K. Bhandari, A. Ghosh, D. ChakrabarƟ, Micromechanics of cleavage fracture and the associated tongue formaƟon in ferriƟc steel, Materials Science and Engineering: A 885 (2023) 145616. hƩps://doi.org/10.1016/j.msea.2023.145616
2023
-
[67]
Shishvan, G
S.S. Shishvan, G. Csányi, V.S. Deshpande, Hydrogen induced fast-fracture, Journal of the Mechanics and Physics of Solids 134 (2020) 103740. hƩps://doi.org/10.1016/j.jmps.2019.103740
2020
-
[68]
Shibata, T
A. Shibata, T. Murata, H. Takahashi, T. Matsuoka, N. Tsuji, CharacterizaƟon of Hydrogen-Related Fracture Behavior in As-Quenched Low-Carbon MartensiƟc Steel and Tempered Medium-Carbon MartensiƟc Steel, Metall Mater Trans A 46 (2015) 5685–5696. hƩps://doi.org/10.1007/s11661-015-3176-x
2015 doi
-
[69]
Cho, P .E
L. Cho, P .E. Bradley, D.S. Lauria, M.L. MarƟn, M.J. Connolly, J.T. Benzing, E.J. Seo, K.O. Findley, J.G. Speer, A.J. SliŅa, CharacterisƟcs and mechanisms of hydrogen-induced quasi-cleavage fracture of lath martensiƟc steel, Acta Materialia 206 (2021) 116635. hƩps://doi.org/10...
2021
-
[70]
Nagao, C.D
A. Nagao, C.D. Smith, M. Dadfarnia, P . Sofronis, I.M. Robertson, The role of hydrogen in hydrogen 29 embriƩlement fracture of lath martensiƟc steel, Acta Materialia 60 (2012) 5182–5189. hƩps://doi.org/10.1016/j.actamat.2012.06.040
2012 doi
-
[72]
Krom, R.W .J
A.H.M. Krom, R.W .J. Koers, A. Bakker, Hydrogen transport near a blunƟng crack Ɵp, Journal of the Mechanics and Physics of Solids 47 (1999) 971–992. hƩps://doi.org/10.1016/S0022-5096(98)00064-7
1999 doi
-
[73]
Y. Qiao, X. Kong, An energy analysis of the grain boundary behavior in cleavage cracking in Fe–3wt.%Si alloy, Materials LeƩers 58 (2004) 3156–3160. hƩps://doi.org/10.1016/j.matlet.2004.05.063
2004 doi
-
[75]
Okada, A
K. Okada, A. Shibata, H. Matsumiya, N. Tsuji, Origin of Serrated Markings on the Hydrogen Related Quasi- cleavage Fracture in Low-carbon Steel with Ferrite Microstructure, ISIJ InternaƟonal 62 (2022) 2081–2088. hƩps://doi.org/10.2355/isijinternaƟonal.ISIJINT-2022-212
2022 doi
-
[76]
Okada, A
K. Okada, A. Shibata, N. Tsuji, CharacterisƟcs and formaƟon mechanism of serrated markings on the hydrogen- related quasi-cleavage fracture in as quenched low-carbon martensiƟc steel, Scripta Materialia 234 (2023) 115568. hƩps://doi.org/10.1016/j.scriptamat.2023.115568
2023
-
[77]
W. Wang, Z. Wang, Z. Sun, Z. Zhou, K. Zhang, L. Ma, Y . Wang, S. Yang, Z. Huang, K. Wang, Study of fractography of ferriƟc ducƟle iron at different temperatures and loading condiƟons, Mater. Res. Express 11 (2024) 016511. hƩps://doi.org/10.1088/2053-1591/ad184a
2024 doi
-
[78]
Chevrier, Experimental Analysis of River PaƩerns in Silicon BriƩle Fractures, J
J. Chevrier, Experimental Analysis of River PaƩerns in Silicon BriƩle Fractures, J. Phys. I France 5 (1995) 675–
1995
-
[80]
Suzudo, K
T. Suzudo, K. Ebihara, T. Tsuru, BriƩle-fracture simulaƟons of curved cleavage cracks in α -iron: A molecular dynamics study, AIP Advances 10 (2020) 115209. hƩps://doi.org/10.1063/5.0026659
2020 doi
-
[81]
Sorbello, P .E.J
F. Sorbello, P .E.J. FlewiƩ, G. Smith, A.G. Crocker, The role of deformaƟon twins in briƩle crack propagaƟon in iron–silicon steel, Acta Materialia 57 (2009) 2646–2656. hƩps://doi.org/10.1016/j.actamat.2009.02.011
2009 doi
-
[83]
Pelligra, J
C. Pelligra, J. Samei, J. Kang, D.S. Wilkinson, The effect of vanadium on microstrain parƟƟoning and localized damage during deformaƟon of unnotched and notched DP1300 steels, InternaƟonal Journal of PlasƟcity 158 (2022) 103435. hƩps://doi.org/10.1016/j.ijplas.2022.103435
2022
-
[84]
M. Kim, A. Lyu, H.-B. Jeong, J.-Y . Lee, Y.-K. Lee, Effect of inclusions on the hydrogen embriƩlement of martensiƟc medium-Mn steel, Journal of Materials Research and Technology 26 (2023) 2724–2736. hƩps://doi.org/10.1016/j.jmrt.2023.08.090
2023 doi
-
[85]
Iwaoka, A
T. Iwaoka, A. Fujiki, Basic Study of High-Copper Containing Steel Scrap Recycle using P/M Process, Journal of the Japan Society of Powder and Powder Metallurgy 58 (2011) 633–639. hƩps://doi.org/10.2497/jjspm.58.633. 30
2011 doi
-
[86]
Schwich, D
H. Schwich, D. Görzen, B. Blinn, T. Beck, W. Bleck, CharacterizaƟon of the precipitaƟon behavior and resulƟng mechanical properƟes of copper-alloyed ferriƟc steel, Materials Science and Engineering: A 772 (2020) 138807. hƩps://doi.org/10.1016/j.msea.2019.138807. Hydrogen-induc...
2020
-
[319]
hƩps://doi.org/10.2355/tetsutohagane.98.311
-
[683]
hƩps://doi.org/10.1051/jp1:1995159
-
[724]
hƩps://doi.org/10.1038/s41467-024-45017-4
-
[1199]
hƩps://doi.org/10.1126/science.aal2418
Reviewed August 15, 2026 · model on record in the stance chip above.